A nanowire LED only works well if its thin indium layer stays put while the wire is grown. NIST scientists have now mapped that layer in three dimensions and found it can be destroyed by growth conditions with no outward sign. The Physical Measurement Laboratory (PML) group made the wires; a technique called laser-assisted atom probe tomography revealed what happened inside.
Why nanowires matter
Semiconductor nanowires are vanishingly small. A recent batch from PML's Quantum Electronics and Photonics Division was about 200 nanometers across and 6 to 10 micrometers long, with embedded layers as thin as 3.3 nm. They are poised to play a large role in solid-state lighting, chemical sensors and nanoscale scientific probes. First, researchers need to learn how to make high-efficiency nanowire light-emitting diodes (LEDs) that are reliably uniform in composition and shape, each with the same emission spectrum and other critical properties. That requires a detailed understanding of how to place different atomic species within the wire and its layers as they form.
The study
Norman Sanford and colleagues in NIST's Optoelectronic Manufacturing Group, with collaborators at the Colorado School of Mines, grew gallium nitride (GaN) nanowires by molecular beam epitaxy, embedding thin layers of indium gallium nitride (InGaN) at intervals. To use such a wire as a light source, a voltage is applied. The InGaN sections form quantum wells that trap electron-hole pairs, and when these recombine they give off light. That is much more efficient than a simple abrupt p-n junction in GaN, but only if the well stays compact and uniform. If indium diffuses into the surrounding regions, the well spreads out, and portions with different indium concentrations have different bandgaps and emit different wavelengths.

Diagram of a nanowire with multiple layers of InGaN embedded during the growth process.
The best growth conditions for the GaN and InGaN segments can differ, so the team made wires over a range of temperatures and molecular-beam properties and examined the effect on the wells with laser-assisted atom probe tomography (L-APT).
How L-APT works
In an ultra-high vacuum chamber at about 54 K, a constant high voltage is applied to a nanowire while pulses from an ultraviolet laser hit its extreme tip. Atoms at the tip ionize and are pulled off by the strong electric field, then fly to a two-dimensional ion detector about 90 mm away. The detector records where each ion lands, and the laser pulses serve as timing signals, so the team can find each ion's time of flight and hence its charge-to-mass ratio. The impacts are mapped back to their origin in the tip, and the accumulated data build a 3D picture of the chemical makeup of every part of the wire.
What it showed
Growth conditions strongly affected how well the InGaN layers stayed localized. If the conditions for the GaN layers grown afterward are not adjusted correctly, indium can diffuse and the InGaN layers disperse. In some cases the layers' consolidation was destroyed during later GaN growth with no obvious outward sign. Wells that stayed localized were thin conical InGaN shells, concentric with the wire, rather than flat discs. According to the group, this is the first time L-APT has been used to examine how growth variations affect such structures, and the results agreed with high-resolution transmission electron microscopy, another technique that reveals composition.
The team also found that changing L-APT settings, such as the laser pulse energy, can give spurious values for the ratio of gallium and indium to nitrogen, a seeming but nonphysical excess of metal. They speculate that high laser pulse energies make neutral nitrogen atoms leave the wire, where the ion detector does not count them.
The hard part: mounting one wire
Handling a single wire this small is uncommonly difficult. A tungsten manipulator probe was welded with platinum to one nanowire, which was placed in a hole in a mounting post and welded in with platinum; then the probe was snapped off, leaving the wire standing upright, ready for L-APT. The greatest challenge, says Sanford, is a mounting scheme that survives the whole analysis without the wire fracturing, because the electric field at the tip is on the order of 10 V/nm, high enough to rip ions off the tip. It took dozens of mounting attempts to obtain the results, and the group is still improving the method.
Even with likely ambiguity in the absolute 3D concentration map of nitrogen, the leader of NIST's Semiconductor Metrology for Energy Conversion project says the 3D mapping of gallium and indium has for the first time given essential information to help guide the growth of these GaN/InGaN nanoscale structures. The study is forthcoming in Physica Status Solidi.
Sources
- National Institute of Standards and Technology, news story "Probing the Inner Secrets of Nanowires" (https://www.nist.gov/news-events/news/2013/12/probing-inner-secrets-nanowires), reporting N.A. Sanford and colleagues, "Laser-assisted atom probe tomography of MBE grown GaN nanowire heterostructures"; one photograph whose caption is not tied to it is left out; rewritten in hubnx's own words.